Grades | Stainless Steels | 00Cr19Ni13Mo3

GB 00Cr19Ni13Mo3

PDF | Word | Print

00Cr19Ni13Mo3 Application:Seamless stainless steel tubes for boiler and heat exchanger

Chemical composition(mass fraction)(wt.%) of the 00Cr19Ni13Mo3
Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.030
Si - 1.00
Mn - 2.00
P - 0.035
S - 0.030
Ni 11.00 15.00
Cr 18.00 20.00
Mo 3.00 4.00

Mechanical properties of grade 00Cr19Ni13Mo3

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
991 (≥) 922 (≥) 34 12 11 Solution and Aging, Annealing, Ausaging, Q+T,etc 324

Physical properties of grade 00Cr19Ni13Mo3

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
375 (≥) 327 (≥) 24 33 31 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
124 882 734 - - -

00Cr19Ni13Mo3 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED