Grades | Stainless Steels | XH55BMTΦK/Ю-BД

GOST XH55BMTΦK/Ю-BД

PDF | Word | Print

XH55BMTΦK/Ю-BД Application:Russia GOCT standard deformation of high temperature alloy grades and chemical composition

Chemical composition(mass fraction)(wt.%) of the XH55BMTΦK/Ю-BД
Elements Min.(≥) Max.(≤) Similar Remarks
C 0.04 0.10
Si - 0.45
Mn - 0.35
P - -
S - -
Cr 9.00 12.00
Ni - remaining
Mo 4.00 6.00
Al 3.60 4.50
Ti 1.40 2.00
Fe - 5.00
Co 12.00 15.50
W 4.50 6.00
V 0.20 0.80
B - 0.020

Mechanical properties of grade XH55BMTΦK/Ю-BД

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
989 (≥) 444 (≥) 11 13 42 Solution and Aging, Annealing, Ausaging, Q+T,etc 344

Physical properties of grade XH55BMTΦK/Ю-BД

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
376 (≥) 469 (≥) 24 41 14 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
711 581 164 - - -

XH55BMTΦK/Ю-BД Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED