Grades | Stainless Steels | Z5CTDV25-15B

AFNOR Z5CTDV25-15B

PDF | Word | Print

Z5CTDV25-15B Application:Stainless steels for general purposes. Plates, wide strips and strips

Chemical composition(mass fraction)(wt.%) of the Z5CTDV25-15B
Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.050
Si - 0.75
Mn - 2.00
P - 0.030
S - 0.015
Cr 13.50 16.00
Mo 1.00 1.50
Ni 24.00 27.00
V 0.10 0.50
Al - 0.40
Ti 1.80 2.30
B 0.0025 0.0080

Mechanical properties of grade Z5CTDV25-15B

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
558 (≥) 611 (≥) 34 44 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 212

Physical properties of grade Z5CTDV25-15B

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
253 (≥) 424 (≥) 12 32 12 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
178 147 835 - - -

Z5CTDV25-15B Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED