Grades | Stainless Steels | 1.4605

AFNOR 1.4605 ( Ferrite )

PDF | Word | Print

1.4605 Application:Stainless steels - Part 2: Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes

Chemical composition(mass fraction)(wt.%) of the 1.4605
Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.030
Si - 1.00
Mn - 1.00
P - 0.040
S - 0.015
Cr 17.00 18.00
Mo - -
Ni - -
Al 1.70 2.10
Ti 4×(C+N)+0.15 0.80

Mechanical properties of grade 1.4605

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
946 (≥) 818 (≥) 42 24 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 341

Physical properties of grade 1.4605

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
794 (≥) 433 (≥) 13 32 34 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
517 592 132 - - -

1.4605 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED