Grades | Stainless Steels | HP 9-4-30

UNS HP 9-4-30 ( Precipitation-Hardening )

PDF | Word | Print

HP 9-4-30 Application:Steel, Sheet, Strip, and Plate 1.0Cr - 7.5Ni - 4.5Co - 1.0Mo - 0.09V (0.29 - 0.34C) Consumable Electrode Vacuum Melted, Annealed

Chemical composition(mass fraction)(wt.%) of the HP 9-4-30
Elements Min.(≥) Max.(≤) Similar Remarks
C 0.29 0.34
Si - 0.10
Mn 0.10 0.35
Ni 7.00 8.00
Cr 0.90 1.10
Al - -
Cu - -
Ti - -
Fe - -
Mo 0.90 1.10
Co 4.25 4.75
V 0.06 0.12
P - 0.01
S - 0.01

Mechanical properties of grade HP 9-4-30

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
355 (≥) 411 (≥) 33 41 22 Solution and Aging, Annealing, Ausaging, Q+T,etc 112

Physical properties of grade HP 9-4-30

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
673 (≥) 499 (≥) 21 42 42 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
133 188 598 - - -

HP 9-4-30 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED