Grades | Stainless Steels | SA-240 S41500

AMS SA-240 S41500 ( Martensite )

PDF | Word | Print

SA-240 S41500 Application:Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications

Chemical composition(mass fraction)(wt.%) of the SA-240 S41500
Elements Min.(≥) Max.(≤) Similar Remarks
C - 0.05
Mn 0.50 1.00
Si - 0.60
P - 0.03
S - 0.03
Cr 11.50 14.00
Ni 3.50 5.50
Mo 0.50 1.00

Mechanical properties of grade SA-240 S41500

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
871 (≥) 387 (≥) 14 22 11 Solution and Aging, Annealing, Ausaging, Q+T,etc 333

Physical properties of grade SA-240 S41500

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
634 (≥) 919 (≥) 11 21 33 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
486 932 519 - - -

SA-240 S41500 Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting