Grades | Stainless Steels | 9Cr18MoV

GB 9Cr18MoV ( Martensite )

PDF | Word | Print

9Cr18MoV Application:Stainless steel bars

Chemical composition(mass fraction)(wt.%) of the 9Cr18MoV
Elements Min.(≥) Max.(≤) Similar Remarks
C 0.85 0.95
Si - 0.80
Mn - 0.80
P - 0.035
S - 0.030
Ni - 0.60
Cr 17.00 19.00
Mo 1.00 1.30
V 0.07 0.12

Mechanical properties of grade 9Cr18MoV

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition HBW
192 (≥) 992 (≥) 41 12 43 Solution and Aging, Annealing, Ausaging, Q+T,etc 434

Physical properties of grade 9Cr18MoV

Property Density
kg/dm3
Temperature T
°C/F
Specific heat
J / kgK
Thermal conductivity
W/mK
Electric resistance
µΩ·cm
292 (≥) 322 (≥) 44 24 24 Solution and Aging, Annealing, Ausaging, Q+T,etc
Temp.
°C/°F
Creep strain limit
(10000h)
(Rp1,0) N/mm2
Creep rupture strength
(10000h)
(Rp1,0) N/mm2
- - -
918 598 152 - - -

9Cr18MoV Range of products
Product type Products Dimension Processes Deliver Status
Plates / Sheets Plates / Sheets 0.08-200mm(T)*W*L Forging, hot rolling and cold rolling Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Steel Bar Round Bar, Flat Bar, Square Bar Φ8-1200mm*L Forging, hot rolling and cold rolling, Cast Black, Rough Turning, Shot Blasting,
Coil / Strip Steel Coil /Steel Strip 0.03-16.0x1200mm Cold-Rolled & Hot-Rolled Annealed, Solution and Aging, Q+T, ACID-WASHED, Shot Blasting
Pipes / Tubes Seamless Pipes/Tubes, Welded Pipes/Tubes OD:6-219mm x WT:0.5-20.0mm Hot extrusion, Cold Drawn, Welded Annealed, Solution and Aging, Q+T, ACID-WASHED